Dusting Concrete Surfaces -- What, why, & how?
|
|
|
WHAT is Dusting?
Formation of loose powder resulting from disintegration
of surface of hardened concrete is called dusting
or chalking. The characteristics of such surfaces are:
- They powder under any kind of traffic
- They can be easily scratched with a nail or even by sweeping
|

Dusting Concrete Surface |
|
|
WHY Do Concrete Floors Dust?
A concrete floor dusts under traffic because the wearing surface is weak.
This weakness is caused by:
- Any finishing operation performed while bleed water
is on the surface or before the concrete has finished
bleeding. Working this bleed water back into
the top 1/4 inch [6 mm] of the slab produces a very
high water-cement ratio and, therefore, a low
strength surface layer.
- Placement over a non-absorptive subgrade or polyethylene
vapor retarder. This reduces normal
absorption by the subgrade, increases bleeding and,
as a result, the risk of surface dusting.
- Floating and/or troweling operations following the
condensation of moisture from warm humid air on
cold concrete. In cold weather concrete sets slowly,
in particular, cold concrete in basement floors. If
the humidity is relatively high, water will condense
on the freshly placed concrete, which, if troweled
into the surface, will cause dusting.
- Inadequate ventilation in enclosed spaces. Carbon
dioxide from open salamanders, gasoline engines
or generators, power buggies or mixer engines may
cause a chemical reaction known as carbonation,
which greatly reduces the strength and hardness of
the concrete surface.
- Insufficient curing. This omission often results
in a soft surface skin, which will easily dust under
foot traffic.
- Inadequate protection of freshly placed concrete
from rain, snow or drying winds. Allowing the concrete
surface to freeze will weaken the surface and
result in dusting.
HOW to Prevent Dusting
- Concrete with the lowest water content with an adequate
slump for placing and finishing will result
in a strong, durable, and wear-resistant surface. In
general, use concrete with a moderate slump not
exceeding 5 inches [125 mm]. Concrete with a
higher slump may be used provided the mixture is
designed to produce the required strength without
excessive bleeding and/or segregation. Water-reducing
admixtures are typically used to increase
slump while maintaining a low water content in the
mixture. This is particularly important in cold
weather when delayed set results in prolonged
bleeding.
- NEVER sprinkle or trowel dry cement into the
surface of plastic concrete to absorb bleed water.
Remove bleed water by dragging a garden hose
across the surface. Excessive bleeding of concrete
can be reduced by using air-entrained concrete, by
modifying mix proportions, or by accelerating the
setting time.
- DO NOT perform any finishing operations with
water present on the surface or while the concrete
continues to bleed. Initial screeding must be
promptly followed by bull floating. Delaying bull
floating operations can cause bleed water to be
worked into surface layer. Do not use a jitterbug,
as it tends to bring excess mortar to the surface.
DO NOT add water
- Do not place concrete directly on polyethylene
vapor retarders or non-absorptive subgrades as
this can contribute to problems such as dusting, scaling,
and cracking. Place 3 to 4 inches [75 to 100
mm] of a trimable, compactible fill, such as a
crusher-run material, over vapor retarders or nonabsorptive
subgrade prior to concrete placement.
When high evaporation rates exist, lightly dampen
absorptive subgrades just prior to concrete placement,
ensuring that water does not pond or collect
on the subgrade surface.
- Provide proper curing by using liquid membrane
curing compound or by covering the surface with
water, wet burlap, or other curing materials as soon
as possible after finishing to retain moisture in the
slab. It is important to protect concrete from the
environment at early ages.
- Placing concrete in cold weather requires
concretetemperatures exceeding 50°F [10°C] as
well as an accelerating admixture.
HOW to Repare Dusting
- Sandblast, shot blast or use a high-pressure washer
to remove the weak surface layer.
- To minimize or eliminate dusting, apply a commercially
available chemical floor hardener, such as
sodium silicate (water glass) or metallic zinc or
magnesium fluosilicate, in compliance with
manufacturer’s directions on thoroughly dried
concrete. If dusting persists, use a coating, such as
latex formulations, epoxy sealers, or cement paint.
- In severe cases, a serviceable floor can be obtained
by wet-grinding the surface to durable substrate
concrete. This may be followed by properly bonded
placement of a topping course. If this is not practical,
installation of a floor covering, such as carpeting or
vinyl tile covering, is the least expensive solution to
severe dusting. This option will require some prior
preparation since adhesives for floor covering materials
will not bond to floors with a dusting problem
and dusting can permeate through carpeting.
|
|
|
Follow These Rules to Prevent Dusting
- Use Moderate slump concrete not exceeding 5 inches [125 mm]
- Do not start finishing operations while concrete is bleeding
- Do not broadcast cement or sprinkle water on concrete prior to or duing finishing operations
- Ensure that there is adequate venting of exhaust gases from gas-fired heaters in enclosed spaces
- Use adequate curing measures to retain moisture in concrete for the first 3 to 7 days and protect it from the environment
|
|
|
References
- Guide for Concrete Floor and Slab Construction, ACI 302.1R.
American Concrete Institute, Farmington Hills, MI.
- Slabs on Grade, Concrete Craftsman Series CCS-1, American
Concrete Institute, Farmington Hills, MI
- The Effects of Various Surface Treatments, Using Zinc and
Magnesium Flusilicate Crystals on Abrasions Resistance of Concrete Surfaces,
Concrete Laboratory Report No. C-819, U.S. Bureau of Reclamation
- Residential Concrete, National Association of Home Builders, Washington, DC.
- Trouble Shooting Guide for Concrete Dusting, Concrete Construction, April 1996.
|
|
|
Back to Tip Index |
|
|